Izingxenye ezimbili, okuqinile okuphezulu, i-zinc phosphate epoxy primer nejazi lokwakha

I-Multi-purpose epoxy primer noma upende ophakathi nendawo wesakhiwo sensimbi nensimbi ethathiwe ezindaweni ezihlukahlukene zomoya.


Imininingwane Yomkhiqizo

Omaka bomkhiqizo

Isingeniso

Izingxenye ezimbili, okuqinile okuphezulu, i-zinc phosphate epoxy primer eyakhiwe nge-epoxy resin, i-zinc phosphate anti-rust pigment, i-solvent, i-ejenti eyisizayo kanye ne-polyamide yokwelapha.

Izingxenye ezimbili, okuqinile okuphezulu, i-zinc phosphate epoxy primer nejazi lokwakha
Izingxenye ezimbili, okuqinile okuphezulu, i-zinc phosphate epoxy primer nejazi lokwakha

Izici

• I-epoxy primer noma ijazi lokwakha ezinhlelweni zokuvikela ezivikelayo
• Ukumelana nokugqwala okuhle kakhulu ekuchayekeni komkhathi
• Yelapha emazingeni okushisa afika ku -5°C (23°F)
• Ubukhulu.ngaphezu kwesikhawu sokumboza akunqunyelwe
• Ukwelapha ngesivinini ekwenziweni kwensimbi
• Ibanga lohlelo olubanzi

Ukusetshenziswa okunconyiwe

I-Multi-purpose epoxy primer noma upende ophakathi nendawo wesakhiwo sensimbi nensimbi ethathiwe ezindaweni ezihlukahlukene zomoya.
Ifanele izinjongo ezintsha zensimbi noma zokulungisa.

Imiyalo yohlelo lokusebenza

Ukwelashwa Okusebenzayo kwe-Substrate kanye Nomphezulu:
Insimbi: ukuqhuma okuhlanzwe ku-Sa2.5 (ISO8501-1), iphrofayela eqhumayo Rz35μm~75μm (ISO8503-1)
Kuyasebenza futhi Ukwelapha:
Izinga lokushisa lendawo ezungezile kufanele libe ukusuka ku-5 ℃ liye ku-38℃, umswakama womoya ohlobene akufanele ube ngaphezu kwama-85%.
Izinga lokushisa le-substrate ngesikhathi sokufakwa kanye nokwelashwa kufanele libe ngu-3 ℃ ngaphezu kwendawo yamazolo.

Impilo yebhodwe

5℃ 15℃ 25℃ 35℃
5 amahora. 4 amahora. 2 amahora. 1.5 amahora

Izindlela zokufaka isicelo

Isifutho esingenamoya/isifutho somoya
I-brush ne-roller coating inconywa kuphela ngejazi lemigqa, ukumbozwa kwendawo encane noma ukuthinta phezulu.
Amapharamitha wohlelo lokusebenza

Indlela yohlelo lokusebenza

Iyunithi

Isifutho esingenamoya

Isifutho somoya

Ibhulashi/Irola

I-Nozzle orifice

mm

0.430.53

1.82.2

—-

Umfutho weNozzle

kg/cm2

150200

34

—-

Mncane

%

010

1020

510

Ukomisa & Ukwelapha

Ukushisa kwe-substrate

5℃

15℃

25℃

35℃

Ingaphezulu-yomile

4 amahora

2 amahora

1 ihora

30 imiz

Ngomile

Amahora angu-24

16 amahora

12 amahora

8 amahora

Isikhawu Sokumboza

Amahora angu-20

16 amahora

12 amahora

8 amahora

Isimo sokumboza Ngaphambi kokufaka ijazi elilandelanayo, indawo engaphezulu kufanele ihlanzeke, yome futhi ingabi nosawoti we-zinc nokungcola.

Ukwandulela & Okulandelayo

Ijazi elandulele:Insimbi eyinsimbi, idiphu eshisayo, isifutho esishisayo esinokwelashwa okungaphezulu kwe-ISO-Sa2½ noma i-St3.I-primer yesitolo egunyaziwe, i-zinc rich primer, i-epoxy primer….
Ijazi elilandelanayo:I-Epoxy, i-polyurethane, i-fluorocarbon... njll.
Akuhambisani nopende we-alkyd.

Ukupakisha & Isitoreji

Usayizi wephakethe:isisekelo 25kg, ukuphulukisa ejenti 2.5kg
Iphuzu elikhanyayo:>25℃(Ingxube)
Isitoreji:Kufanele igcinwe ngokuhambisana nemithetho kahulumeni wendawo.Indawo yokugcina impahla kufanele yomile, ipholile, ingene umoya futhi iqhelelane nokushisa nemithombo yomlilo.Ibhakede kufanele ligcinwe livalwe ngokuqinile.